Plastication: 50 to 65rpm
Injection Pressure: Set to give 6 to 10 seconds injection time
Hold Pressure: 50 to 100% of injection pressure
Hold Time: 15 sec minimum
Cure Time, 0.125 in: 40 to 45 sec
Water Absorption, ASTM D570, 48 hrs, 50°C: 2.2%
Dielectric Strength, ASTM D149, 60 Hz, Method A, wet: 140 V/mil
Dielectric Strength, ASTM D149, 60 Hz, Method B, wet: 80 V/mil
Bulk Factor, ASTM D1895: 3.6 to 4.6
Compression and Transfer Molding Conditions:
- Preforming Pressure: 8000 to 12000 psi
- Preheat Temperature: 210 to 235 °F
- Mold Temperature: 330 to 360 °F
- Compression Mold Pressure: 2500 to 5000 psi
- Transfer Mold Pressure: 4000 to 6000 psi
- Cure Time, 0.125 in: 40 to 50 sec