Veromor® Purge Processing Procedure
Mix 20% Veromor® Purge with medium flow HDPE, polypropylene or the polymer you plan to process next.
Starve screw & barrel.
Temperature: Purge between 200-300°C. Lower temperatures can be used. Ensure carrying polymer will flow through equipment at the lower temperatures. Polymer will be stiffer when mixed with Veromor® Purge
RPM: You do not need to adjust the RPM in most cases prior to purging. It is recommended that the amp meter be observed to ensure purge is flowing satisfactorily through the barrel.
Add Veromor® Purge polymer/purge mix to hopper & process through equipment.
For Hot Runner Systems: Add 1 - 2 kg (2.2 - 4.4 lb) of Veromor® Purge -XR polymer/purge mix for every 25mm (1 inch) barrel diameter.
Flush out Veromor® Purge with polymer you plan to process next.
Note: If the screw & barrel have very bad carbonization, increase amount of Veromor® Purge processed through the barrel.
Veromor® Purge can be used at higher addition level, must not exceed 35%.
Veromor® Purge -XT and Veromor® Purge -XS are not suitable for hot runner systems.
|
|
Product names can be difficult to match. You may have searched any one of these terms to find this product: Veromor® Purge -XR, Veromor Purge XR, Veromor® Purge , Veromor Purge, VeromorPurgeXR, VeromorPurge, Purge-XR, PurgeXR, Purge:XR, Purge/XR, Purge+XR, Purge_XR, Purge XR, Purge, -XR, XR, :XR, /XR, +XR, _XR, XR, Proprietary, PlastxWorld, XRPurge
|